When inspecting the rust and cracks on the side plate of the excavator boom, it is necessary to scrape off or polish the paint layer and rust on the surface of the weld. When observing, use a small hammer to lightly tap the weld, and if necessary, use a magnifying glass to observe.
1. Reasons for crack formation
The reasons for cracks on the side plate of the excavator boom include: bubbles, slag inclusions, and small cracks in the original weld seam itself. When the excavator is overloaded, small cracks will appear at the original weld seam and gradually expand. Cracks will occur due to the mismatch between the performance of the welding rod and the plate during welding. Due to the large volume of the excavator boom, it is difficult to use reliable and effective heating and insulation measures. After welding, the hardened area of the base material around the weld seam cannot be completely removed, resulting in a decrease in weld strength. During the operation of the excavator, the vibration impact is large, and the uneven stress at the weld seam causes the weld seam to crack.
2. Repair method
Preparation before welding: Use a hand grinding wheel to clean the oil stains, paint, rust, etc. at the crack of the original weld seam. Use an air planer to cut off the cracks in the weld seam to the body of the side plate, and remove the hardened area of the base material that was previously welded. After cutting, use a corner grinding wheel to smooth the incision (with a V-shaped groove on the inner interface). After cleaning and pink inspection, confirm that all cracks have been found and removed completely.
According to the existing maintenance conditions, use E5015 (J507) or E5016 (J506) welding rods with a diameter of 5mm, bake at 350 ℃ for 2 hours, and then keep warm at 100 ℃ to prevent the welding rods from absorbing moisture. They can be used as needed; Welding current 190-230A. Due to the large thickness of the excavator side panel, the welded area should be preheated to 150-250 ℃ before welding; During the welding process, segmented, symmetrical, and reverse welding methods can be used; During the cooling process of the weld seam, the weld metal should be continuously struck with a hammer to eliminate stress; When welding at the corner of the side panel, continuous welding is recommended to avoid arc defects and improve the stress condition at the connection.
After welding, thoroughly remove spatter, welding slag, and weld beads, and the weld seam height should not exceed 2.5mm. Perform magnetic particle inspection on the weld seam, and no defects such as cracks are allowed.
3. Measures to prevent weld corrosion
Thoroughly polish, remove rust, and apply anti rust paint to the weld seam. At the excavation construction site, for existing corroded welds, manual rust removal can be chosen based on the actual situation. The disadvantage is that the labor intensity of workers is relatively high and the labor cost is high; Acid pickling can also be used for rust removal, which is mainly based on organic acids, combined with composite materials such as corrosion inhibitors, surfactants, rust removers, rust inhibitors, and film-forming agents, to prepare an acid pickling solution with rust removal, rust prevention, and primer functions. The purpose of rust removal and rust prevention is achieved through cleaning.
In addition, during use, attention should be paid to keeping the excavator in a clean and dry environment, maintaining good ventilation, and promptly eliminating corrosive gases and moisture.
Repair of excavator boom
Oct 17, 2024
You May Also Like
Send Inquiry
Categories
Contact Us
- Tel: +8613021788885
- Email: hengtongtrailer@163.com
- No. 29 Liangshan Industrial Park, Liangshan County, Shandong Province